Greensand: A New Chapter
Faced with the idea of making new plaster molds and worrying about how they can crack during the wax burnout in the kiln, we thought we should stop using plaster and learn how to make greensand molds. While plaster and silica can work for bronze, we'll need greensand molds for iron anyway, so why not start now?
We've been working on this new technology for a couple of months now - there's lots to learn. First, we had to make the frames. These are essentially two identical wooden frames that should sit together perfectly tight. The top is called the cope and the bottom, the drag.
In our development of the Fire Craft, we always like to try making things ourselves as much as possible, and it turns out you can make decent greensand with play sand and bentonite sourced from some types of kitty litter—ones made of nothing but clay. (Bentonite is very absorbent, so kitty litter uses bentonite.)


But no. The sand stayed stuck around the bow and "lip" of the pattern, probably because those areas are undercut and angled sharply against the pillar part. The rest of the pattern looked pretty good though! So at one level we were happy that the sand is working, and does seem to retain its shape well. You can imagine molten bronze flowing in there no problem. (Well, we'd like to imagine.)
So, we put the kitty litter in our blender and ground it up as fine as possible. And then mixed it very thoroughly into our sifted play sand so it was about 10% of the whole. Spraying it slowly and minimally with water, we continued mixing until we felt it was "right." One way to test is to squeeze a handful of it and if the sands molds your fingers and holds and then breaks evenly when bent, it's basically there. In the photo below, it looks a little too wet (and we'll see why that matters later).


You actually want the sand to be pretty dry, drier than you might imagine. What creates the bond are all the tiny particles of bentonite that swell up so much in between the sand particles, and those don't need a lot of water to become "sticky."
So, once we thought the sand was right (and remember, we don't really know anything about what we're doing; this is all learn as you go), we started to try to mold our patterns. We had a Venus, a salamander and also a yoni-lingam.
Essentially, you're trying to make a two-part mold of your object, with the sand for each half packed into the top and bottom frames (the cope and the drag). We set our drags on a flat work surface and then embedded our patterns halfway, horizontally, in a bed of greensand. Then we rammed the sand hard, pounding it with a rammer. Next, we gave the whole thing a light dusting of parting dust (flour, talc, etc.), placed the cope on top of the drag, and started adding greensand to cover the figure entirely.
You want to go lightly with the sand at first so it falls all over the pattern, filling all the cavities and capturing all the details. Once the cope was full of sand, we again rammed it all over. The greensand gets compressed very nicely and packed in all over the figure within.
After ramming, and once you strike all the excess sand off, you've basically got your mold.
Since we were just experimenting with the greensand, we didn't really make proper molds with sprues and such. Nor did we properly finish the frames with registration pins or locks to make sure the cope and drag are perfectly aligned. We just wanted to see if the sand would work and get us a good Side A and Side B.
I lifted the cope off of mine gently gently, to see if it worked...
Nope! The whole thing fell apart. I probably hadn't rammed it all hard enough but the main problem was I had filled my frames with sand from the wrong container, using way too much regular sand and not greensand. Next, Jorge pulled his cope off to reveal a Venus...
which was embedded in greensand that was a little too... moist. Looks like he'd used too much water when making the mix and it was all a bit too muddy. But one very nice thing about working with greensand is that it's super easy to start over. So he did, with a better greensand mix and this time:
I tried again too, this time with a pewter yoni-lingam, thinking that it might separate from the sand better than plastic resin does. I put it into the drag, halfway, and rammed the sand in nice and tight.
And then the moment of truth...
So, for the next attempt we've decided to fill in the bowl of the object with wax and make the edges against the pillar less sharp, more sloped. Hopefully, that will solve the problem.